What is the correct solder and flux to use for refacing a recoil escapement with an offcut of mainspring?

As an experiment I've tried soft soldering using plumbers Plowerflow and lead-free solder with brass and that is fine, however the results on steel are hopeless; the solder just doesn't flow.

I believe you are supposed to use a tin/lead solder, but I'm not sure on what flux you should use.

 

Link to comment
Share on other sites

If you use a 60/40 tin lead solder, then the best flux to use is a zinc chloride flux. You could even use it neat and not diluted. Rinse well after, as it is highly corrosive. All not very environmentally friendly, but in the qtys you will be using, I think you should be OK

Link to comment
Share on other sites

26 minutes ago, Watcher said:

Yet another useless comment from this moderator!

I put bog standard tin of flux because It wasn't anything special.  I can’t remember the name as I never bought it. Did you really want me to have put all that down? 

Link to comment
Share on other sites

"Bog standard" is not an offensive phrase. What's the problem?
It's a phrase that simply conveys that something is very common.
Why am I getting reports regarding that?

Sent from my SM-G950F using Tapatalk

Link to comment
Share on other sites

Oldhippy may be a Moderator but he knows more about timepieces than most of us put together!

I wish I had as much technical help to offer  the good people on this site as he does! Even 1/10th of his horology wisdom.  Instead I stumble around giving my thoughts on what sharpening stone is the best, and mundane information like that. Or deciding weather this word or that word is politically correct?

We have to be more civil in this world of  barbarians world we live in today.

  • Like 2
Link to comment
Share on other sites

When I did this recently I used tin / lead solder.

I have a big bar of it that would of been for repairing car radiators that I just hit flat with a hammer until its very thin and then just snip a bit off.

For flux I uses Bakers flux that you should be able to buy at any hardware store which as said above is zinc chloride flux.

In the old days you made it by dropping Zinc into hydrochloric acis until it stopped fixxing and used the link which was Zinc Chloride.

Now you just buy a bottle of it ready made, much easier.

As said make sure you clean up after soldering it it will rust the part

Link to comment
Share on other sites

Preparation is necessary. I would use a fine emery stick to clean the pallet face and to clean of all the blue on the spring that is to be used. Make sure both are free from oil and grease. I used a spirt lamp with a medium flame. You need enough solder which must be even to cover the pallet face otherwise it will not lay flush to the face. This will affect the action. If repaired correctly you will not be able to tell the pallets have been re-faced.    

I thought this might help you.

Link to comment
Share on other sites

I agree with what oldhippy says, if its not perfectly clean it wont solder properly, and dont forget to scuff up the back of the spring material with some W&D, then flux and tin both parts before trying to solder them together

Link to comment
Share on other sites

  • 3 weeks later...

Well I just wanted to feed back on this now I've changed my flux and solder.  I have obtained some "Bakers Fluid No 3" and 60/40 tin/lead solder.

I found that applying flux, holding together, then applying solder wasn't successful like you might do with silver soldering.  

I did however find that tinning both surfaces first (having cleaned as suggested above) and then soldering together resulted in a good joint that when cleaned up didn't show any join.

Link to comment
Share on other sites

Join the conversation

You can post now and register later. If you have an account, sign in now to post with your account.
Note: Your post will require moderator approval before it will be visible.

Guest
Reply to this topic...

×   Pasted as rich text.   Restore formatting

  Only 75 emoji are allowed.

×   Your link has been automatically embedded.   Display as a link instead

×   Your previous content has been restored.   Clear editor

×   You cannot paste images directly. Upload or insert images from URL.



  • Recently Browsing

    • No registered users viewing this page.
  • Topics

  • Posts

    • Showing state of hairspring on receipt, backplate & 'dished' wheel. 
    • I would harden and temper (to a light blue). It's so easy to do and only takes a couple of minutes. A search on ebay UK for "spring steel strip cs" finds plenty available in small quantites and thicknesses from 0.1mm up.  But the question is ( @nickelsilver) which "CS" number is best for watch parts ?  Also, from one of the ads : "CARBON SPRING STEEL. SIZE IS METRIC 15.00mm X 0.10mm X 304 MM  CS100 FINISH BRIGHT . HARDENED AND TEMPERD TO 480-530VPN" I've no idea about 480-530VPN. Does that mean it needs annealing before working?       Have you seen this video, he shows how to determine where the indents go ?  
    • Here is the insert ring for rectangular or elliptical movements: Note that the length is the side with the stem cut out on the spreadsheet (in the picture below this is 15.15: Here is the fake pdf file, again you need to convert to .zip after download to access the FreeCAD and 3mf files. Rectangular insert disc.pdf    
    • as you took the mainspring out what did it look like? It's amazing how much amplitude you can get if the mainspring actually has the proper shape. last week I was doing a 12 size Hamilton and was very much surprised with the beautiful back curvature the mainspring had. Then the watch had a really nice amplitude the group would be so proud it was 350 until I dropped the lift angle down to 38 that drop the amplitude quite a bit below 300. then with the beautiful back curve it still had really nice amplitude the next day. I really wish all my mainspring's look like this as the watch had beautiful amplitude the next day. So many of the aftermarket pocketwatch Springs I see now do not have anything resembling a back curve may be a slight curve and that's about all. They still work but they just don't work as nice as a properly made spring. then Omega as all sorts of nifty technical documentation unfortunately every single corner is watermarked with where it came from who downloaded it etc. very paranoid company. On the other hand I will snip out images like from the document on recycling a mainspring barrel. for instance here's the section on what your mainspring should look like. water damaged a lot of times means rust was there rust on this watch?
×
×
  • Create New...